ALUMINUM OXIDE 2N5
Chemical formula: Al2O3
Chemical purity: 2N5
Mechanical Properties:
Density g/cc (#/in3): 3.89 (0.14)
Surface Finish - CLA: Micrometers Microinches
As-Fired: 0.9 35
Ground: 0.5 20
Polished: 0.1 3.9
Crystal Size:
Range: 5-50 197-1970
Average: 17 670
Water Absorption Percent: 0
Gas Permeability: 0
Color: Ivory
MPa psi × 103
Flexural Strength (Mor) at 20 oC: 379 55
GPa psi × 106
Elastic Modules at 20 oC: 372 54
Shear Modules at 20 oC: 152 22
Bulk Modules at 20 oC: 228 33
m/sec. ft/sec.
Trans. Sonic Vel. at 20 oC: 9.8 × 103 32 × 103
Poisson's Ratio at 20 oC: 0.22
Stiffness/Weight at 20 oC (GPa/g/cc): 96
Fracture Toughness at KIC (MPA ⋅ m 1/2): 4-5
MPa kpsi
Compressive Strength at 20 oC: 2620 380
Tensile Strength: at 25 oC: 262 38
at 1000 oC:
GPa kg/mm2
Hardness: Knoop 1000 g: 14.1 1440
Rockwell 45N: 83
Thermal Properties:
W/m oK Btu⋅in/ft2⋅h⋅ oF
Thermal Conductivity at 20 oC: 35.6 247
10-6/ oC 10-6/ oF
Coefficient of Thermal Expansion at 25-1000 oC: 8.2 4.6
J/kg⋅ oK cal/g⋅ oC
Specific Heat at 100 oC: 880 0.21
oC oF
Thermal Shock Resistance, ΔTc: 200 392
Maximum use temperature: 1750 3182
Electrical Properties:
Dielectric Strength: ac-kv/mm ac-volts/mil
at 6.35 mm: 8.7 220
at 3.18 mm: 11.4 290
at 1.27 mm SPEC: 16.9 430
at 0.64 mm Thick: 22.8 580
at 0.25 mm: 33.1 840
1 kHz 1 MHz 1 GHz
Dielectric Constant at 25 oC: 9.8 9.7 9.7
Dissipation Factor at 25 oC: 0.0002 0.0003 0.0002
Loss Index at 25 oC: 0.002 0.003 0.002
Volume Resistivity: ohm-cm2/cm
at 25 oC: >1014
at 300 oC: 1.6 ×1013
at 500 oC: 2.1 × 1010
at 700 oC: 4.4 × 108
at 1000 oC:
oC oF
Te Value:
Wear Chemical Properties:
Corrosion Resistance - Weight Loss: mg/cm2/day
95% H2SO4 at 20 oC: 0.01
95% H2SO4 at 100 oC: 0.1
Impingement: 0.47
Rubbing: